Research spotlight: Fatemeh Zahra Akbarzadeh

9 min read13 views

At a glance

A Corrosion Science study shows that tuning AZ91 magnesium's microstructure before electrodepositing hydroxyapatite produces a near defect-free coating and a sevenfold rise in polarization resistance.

a rusted metal surface with blue and yellow paint
Photo by Zsolt Palatinus on Unsplash

A coating on a magnesium bone screw is only as good as the metal sitting under it. That sounds like a truism, but until recently nobody had mapped the link with much precision — and a team working between Iran and Belgium has now put numbers on it. By heat-treating an AZ91 magnesium alloy before electrodepositing a hydroxyapatite layer, they raised the polarization resistance of the starting cast alloy roughly sevenfold, a direct measure of how strongly a surface resists the electrochemical reactions that dissolve it.

The work appears in Corrosion Science (volume 245, article 112678) and was led by Fatemeh Zahra Akbarzadeh of the Department of Materials Engineering at Babol Noshirvani University of Technology, with Mohammad Rajabi and Roohollah Jamaati at the same department and Annabel Braem at KU Leuven's Department of Materials Engineering. The argument is simple to state and laborious to prove: the microscopic arrangement of a magnesium alloy's second phases decides how a calcium phosphate coating grows, where it fails, and how long it protects.

Why now matters. Magnesium implants have moved from lab curiosity to regulated product. Compression screws made of magnesium alloys have held European approvals since 2013, and bioresorbable scaffolds and biliary stents followed. All of them depend on a degradation rate slow enough to hold a fracture together and fast enough to vanish afterwards. Coatings are the main lever for that timing. The paper suggests the lever has a second handle that process engineers have largely been ignoring.

Three versions of the same alloy, one plating bath

AZ91 is a workhorse casting grade: magnesium with 9.6 wt% aluminium, 0.86 wt% zinc and 0.13 wt% manganese, with iron, nickel and copper kept down to trace levels. Its microstructure is not uniform. A matrix of nearly pure magnesium, called the alpha phase, is interrupted by a harder intermetallic, the beta phase or Mg17Al12, which in cast metal sits as coarse slabs and networks along grain boundaries. Small Al8Mn5 particles form as well, because of the manganese.

Hydroxyapatite is the calcium phosphate mineral that makes up most of the inorganic fraction of bone and teeth, with the formula Ca10(PO4)6(OH)2. Coating a metal with it does two jobs. It presents a surface that bone cells recognise, and it separates reactive magnesium from body fluid for as long as the layer holds.

The team cut discs six millimetres thick and 170 square millimetres in area, then built three sample groups. One was left as cast. The second was solution-treated at 420°C for 16 hours under argon and water-quenched, a schedule designed to dissolve the beta phase completely. The third received the same solution treatment plus two hours at 350°C, an aging step intended to re-precipitate beta as fine particles inside the grains rather than as thick walls along their edges.

Grain size barely budged: measurements landed between 41.7 and 48.3 micrometres across all three conditions. Whatever changed the corrosion behaviour, it wasn't grain refinement.

Every group then went through an identical electrodeposition bath containing calcium nitrate tetrahydrate, ammonium dihydrogen phosphate and hydrogen peroxide. Electrodeposition is the least glamorous of the calcium phosphate coating methods and that is exactly why it gets used: it runs at room temperature in a water-based bath, the sample acts as the cathode, and an applied voltage drives calcium and phosphate ions to the surface where they precipitate. Finally the samples were tested electrochemically in simulated body fluid, a salt solution formulated to mimic the inorganic composition of blood plasma.

The battery inside the metal

The beta phase holds far more aluminium than the surrounding matrix, and that compositional gap creates a voltage gap: roughly minus 1.71 volts for the alpha phase against minus 1.00 volts for beta. Drop the alloy into salt water and every beta particle becomes the cathode of a microscopic battery, with the neighbouring magnesium playing anode and dissolving away. Multiply that by millions of particles and you have the alloy's corrosion behaviour in miniature.

Picture a steel plate studded with tiny copper rivets, left out in the rain. The rivets don't corrode; the steel around them does, and it corrodes fastest right where the two metals touch. That is micro-galvanic corrosion, and in AZ91 the rivets are the beta particles and the Al8Mn5 inclusions.

What this study adds is the placement of that micro-battery in the chain of events that produces a coating. Immersed in the plating bath, AZ91 does not wait passively for calcium phosphate to arrive. It reacts first, growing a magnesium hydroxide film, Mg(OH)2. The thickness and uniformity of that film set the local current density during deposition and control how much Mg2+ escapes into the electrolyte. Both factors govern where hydroxyapatite nucleates and how its crystals grow.

Because the beta phase determines how evenly the hydroxide forms, it also determines the coating above it. On aged samples, where beta sat as fine precipitates inside the grains, the hydroxide layer came out fine and the hydroxyapatite followed. On as-cast metal, with coarse beta strung along grain boundaries, the coating developed defects concentrated over the regions where alpha and beta sit together in eutectic lamellae.

The authors are blunt about this causal chain. They write that "the substrate microstructure directly impacts the nucleation and growth of coatings, the formation of intermediate layers, and the overall corrosion behavior." The paper's stated gap in the literature was that the relationships between substrate microstructure and electrodeposited coatings "remains largely unexplored" — a claim that holds up when you look at how much of the coating literature treats the substrate as a passive slab.

a close up of an orange and yellow substance

Photo by Eric Prouzet on Unsplash

What the numbers actually say

The best coating came from the simplest treatment. Solution-treated AZ91 produced a nearly defect-free, uniform hydroxyapatite layer and the lowest corrosion current of the three groups. Coated as-cast samples carried their defects into the test and drew higher corrosion currents, which is the electrochemical signature of electrolyte reaching bare metal through pinholes. Comparing the two endpoints — bare as-cast alloy at the start, solution-treated plus coated alloy at the finish — polarization resistance rose about sevenfold.

Heat treatment on its own helped too, though less dramatically. Before any coating, the corrosion rate of the cast alloy fell 22% after solution treatment and 12% after aging. The authors attribute this to two effects: fewer cracks forming in the corrosion product layer, and passivation encouraged by calcium carbonate forming on the surface.

One result deserves a second look because it runs against intuition. Aging produced the finest beta precipitates, and it produced the finest hydroxyapatite morphology. Yet the solution-treated substrate, where beta had been dissolved away entirely, gave the more protective coating. Fineness of coating and protective quality are not the same variable, and the paper is careful to report them separately rather than folding them into a single story about smaller meaning better.

The gap between a salt solution and a femur

Simulated body fluid is a test-tube approximation. It carries the inorganic ions of blood plasma and none of its biology: no proteins competing for the surface, no cells remodelling the interface, no mechanical load cycling through the implant. A coating that survives an electrochemical sweep can still craze during screw insertion, or degrade on a different schedule once macrophages arrive at the wound site. The paper's claims sit inside that boundary.

The scope is also narrow by design. One alloy grade, one solution-treatment schedule, one aging condition. Whether other hold times at 350°C would beat the ones reported here is untested in this paper. A companion study from the same group, published in Surfaces and Interfaces in 2024, ran a time series of solution treatments at 420°C and found that eight hours produced the thinnest and most uniform hydroxide film and the finest hydroxyapatite. The Corrosion Science paper asks a different question: what happens when you add an aging step and change where the beta phase sits.

Aluminium is a separate reason for caution. AZ91 carries nearly ten percent of it, and long-term aluminium release from a resorbing implant has been a recurring worry in the biomaterials literature — one reason clinical devices have tended toward Mg-Y-RE, Mg-Zn-Ca and high-purity magnesium rather than high-aluminium casting grades. A good coating slows the release. It does not change what the substrate is made of.

Independent reviews of biodegradable magnesium make a related point from the clinical side. The field still lacks standardised protocols for comparing in-vitro degradation data across labs, and correlation between bench tests and animal outcomes is weak enough that a result like this one needs replication in more physiological setups before anyone writes it into a device specification.

A furnace schedule as a coating specification

For manufacturers, the useful translation of this paper is that a heat treatment becomes part of the coating recipe. Sixteen hours at 420°C is a long, energy-hungry step, and any plant adopting it has to weigh furnace time against the cost of scrap from patchy coatings. The offsetting argument is that nothing else in the process changes: no new plating chemistry, no vacuum equipment, no rare-earth alloying additions. The deposition itself stays a room-temperature bath.

The clinical stakes are easy to state. Magnesium's elastic modulus, somewhere around 35 to 45 gigapascals, sits far nearer cortical bone than the roughly 110 gigapascals of titanium alloy, so a magnesium plate shares load with the bone instead of shielding it from stress. Magnesium ions released as the implant dissolves have been linked to osteoblast activity. Reviews of the field put the target degradation rate for orthopaedic use under about half a millimetre a year, which is exactly the kind of figure a uniform coating can deliver and a patchy one cannot.

Read alongside each other, the anatomy of the result is a supply-chain point as much as a metallurgical one. Casting houses produce AZ91 to a composition specification, not a microstructure specification. If coating performance depends on where the beta phase sits, then foundries and coating lines have a conversation to have about heat treatment as a shared process step rather than an afterthought at the plating shop.

What to watch over the next five years

Two kinds of follow-up work would move this from a lab observation to a line item in a device file. The first is adhesion and cell-culture testing on heat-treated substrates, because a coating that spalls under torque is worse than no coating at all. The second is animal studies where the layer has to survive real loading and real inflammation, not just a potentiostat sweep.

There is also a design principle here that travels beyond magnesium. Surface engineers have spent decades tuning bath chemistry, current density and deposition time. This paper argues that the substrate is a variable in the same equation, and in AZ91's case the most consequential one. On a screw thread or a stent strut, where coating thickness varies with local geometry, getting the metal's phase structure right first may be the cheapest uniformity tool available.

  • materials-engineering
  • biomaterials
  • electrodeposition
  • az91-magnesium-alloy
  • hydroxyapatite-coating
Portrait of Jarrod Kanizay
About the author

Jarrod KanizayView author

Academic Jobs In House Author

Visionary leader transforming academic recruitment with 20+ years in higher education.

Acknowledgements:

Discussion

Sort by:

Be the first to comment on this article!

You

You’ll be asked to sign in before your comment is posted.

Browse by Faculty

Browse by Subject

Frequently Asked Questions

🔬What did this study actually discover?

The team found that changing the microstructure of an AZ91 magnesium alloy before coating it changes both the shape of the electrodeposited hydroxyapatite layer and how well that layer protects the metal. Solution-treated AZ91 produced a nearly defect-free, uniform coating with the lowest corrosion current. The polarization resistance of the as-cast alloy rose about sevenfold after solution treatment followed by hydroxyapatite coating.

⚙️What is AZ91 magnesium alloy and why use it for implants?

AZ91 is a casting alloy of magnesium with about 9.6 wt% aluminium, 0.86 wt% zinc and 0.13 wt% manganese. It is cheap, casts well and has an elastic modulus far closer to bone than titanium's, which reduces stress shielding. Its microstructure contains an alpha magnesium matrix, a beta phase (Mg17Al12) and small Al8Mn5 particles. The paper studies how that internal arrangement affects coatings.

🦴What is hydroxyapatite and why coat a metal with it?

Hydroxyapatite, Ca10(PO4)6(OH)2, is the calcium phosphate mineral that forms most of the inorganic part of bone and teeth. A hydroxyapatite coating gives an implant a surface bone cells recognise and creates a physical barrier between reactive magnesium and body fluid. The paper uses electrodeposition to form it because that method runs at room temperature in a water-based bath.

🔥Why heat-treat the alloy before coating it?

Heat treatment relocates the beta phase. Solution treatment at 420°C for 16 hours dissolves it completely; a following two-hour aging step at 350°C re-precipitates it as fine particles inside the grains. Because beta particles act as cathodes in micro-galvanic corrosion, their size and position control how evenly the magnesium hydroxide intermediate layer forms, and that layer shapes the hydroxyapatite coating above it.

📈What is polarization resistance and why does sevenfold matter?

Polarization resistance, abbreviated Rp, measures how hard it is to drive an electrochemical reaction at a metal surface. A higher value means the surface resists dissolution. The paper reports that Rp for the initial as-cast alloy increased roughly sevenfold after solution treatment followed by hydroxyapatite coating, which is the headline protective gain of the study.

📉How much did heat treatment alone reduce the corrosion rate?

For the uncoated alloy, the corrosion rate fell 22% after solution treatment and 12% after aging. The authors attribute this to fewer cracks forming in the corrosion product layer and to passivation encouraged by calcium carbonate forming on the surface. Notably, the finer beta precipitates produced by aging did not give the best protection once a coating was applied.

🔋What is micro-galvanic corrosion?

When two phases in an alloy have different electrode potentials, they form tiny batteries on the metal surface. In AZ91 the alpha phase sits near minus 1.71 volts and the beta phase near minus 1.00 volts, so beta acts as a cathode and the surrounding magnesium dissolves as the anode. The Al8Mn5 particles behave the same way. The result is uneven dissolution that carries through into uneven coating growth.

🧪What is simulated body fluid and what are its limits?

Simulated body fluid is a laboratory salt solution that approximates the inorganic ion content of blood plasma. It is standard for electrochemical corrosion testing but contains no proteins, no cells and no mechanical loading. Results in it are useful for ranking materials and for mechanistic work, not for predicting how a coated implant will behave in living bone. The paper's conclusions are framed within that boundary.

🏥Is this coating ready for patients?

No. The study is an in-vitro electrochemical and microstructural investigation on a single alloy grade with one solution-treatment schedule and one aging condition. Adhesion under insertion torque, cell response, and degradation in living tissue were not part of the experimental design. Clinical magnesium devices already exist, but they use different alloys and different surface strategies.

📄Where can I read the full paper?

The article is 'Microstructural tuning of AZ91 magnesium alloy for improved morphology and corrosion protection of electrodeposited hydroxyapatite coatings' by Akbarzadeh, Rajabi, Jamaati and Braem, published in Corrosion Science volume 245 (2025), article 112678. It is available through Elsevier at its DOI, and a record is held in KU Leuven's Lirias repository.

🏭What does this mean for people who make implant coatings?

It reframes heat treatment as part of the coating specification rather than an upstream metallurgical detail. If coating uniformity depends on where the beta phase sits, then foundries and plating lines need a shared process step. The trade-off is furnace time against scrap from defective coatings; the advantage is that bath chemistry, equipment and deposition temperature stay unchanged.

💰Who funded the research and were there conflicts of interest?

The publicly accessible portions of the article record do not list a specific grant or funding body. In the group's related 2024 paper in Surfaces and Interfaces, on the same alloy system, the authors state that they have no known competing financial interests or personal relationships that could have appeared to influence the work.